ANALISIS EKSTRAKSI BIJIH EMAS PT. ANTAM Tbk. SITE ARINEM DENGAN METODE PULVERIZED BOTTLE ROLL TEST MENGGUNAKAN REAGEN FLORREA GOLDIX 570

ASWORO, MONIKA (2023) ANALISIS EKSTRAKSI BIJIH EMAS PT. ANTAM Tbk. SITE ARINEM DENGAN METODE PULVERIZED BOTTLE ROLL TEST MENGGUNAKAN REAGEN FLORREA GOLDIX 570. Other thesis, UPN "Veteran" Yogyajarta.

[thumbnail of 1. Skripsi Fulltext_116180005_Monika Asworo.pdf] Text
1. Skripsi Fulltext_116180005_Monika Asworo.pdf
Restricted to Repository staff only

Download (5MB)
[thumbnail of 2. Cover_116180005_Monika Asworo.pdf] Text
2. Cover_116180005_Monika Asworo.pdf

Download (135kB)
[thumbnail of 3. Abstrak_116180005_Monika Asworo.pdf] Text
3. Abstrak_116180005_Monika Asworo.pdf

Download (226kB)
[thumbnail of 4. Lembar Pengesahan_116180005_Monika Asworo.pdf] Text
4. Lembar Pengesahan_116180005_Monika Asworo.pdf

Download (236kB)
[thumbnail of 5. Daftar Isi_116180005_Monika Asworo.pdf] Text
5. Daftar Isi_116180005_Monika Asworo.pdf

Download (335kB)
[thumbnail of 6. Daftar Pustaka_116180005_Monika Asworo.pdf] Text
6. Daftar Pustaka_116180005_Monika Asworo.pdf

Download (456kB)

Abstract

iv
ABSTRAK
Dalam proses pengolahan emas, merkuri dan sianida merupakan reagen
pelindian emas yang memiliki efek toksik yang berbahaya bagi lingkungan dan
makhluk hidup didalamnya. Florrea Goldix 570 adalah salah satu reagen
pelindian emas dan perak yang ramah lingkungan yang diharapkan dapat
menggantikan sianida. Penelitian ini bertujuan untuk menganalisis karakterisasi
mineral bijih emas, menganalisis pengaruh konsentrasi reagen dan distribusi
ukuran butir terhadap persen ekstraksi emas dengan metode menggunakan reagen
Florrea Goldix 570.
Material yang digunakan merupakan tipe vein yang memiliki karakteristik
partially oxidised atau sebagian teroksidasi dengan dominasi tipikal sulfidis,
berasal dari PT. Antam Tbk. Site Arinem. Penentuan kadar emas (head grade)
dilakukan dengan fire assay, komposisi kimia bijih menggunakan ICP serta
kandungan karbon dan sulfur menggunakan LECO analysis. Penentuan
karakterisasi komposisi mineral dominan dilakukan dengan pengujian
menggunakan XRD dan pengujian mineragrafi dilakukan dengan menggunakan
mikroskop optik. Penelitian dilakukan pada kondisi konsentrasi reagen pada 300,
600 dan 1000 ppm, ukuran distribusi umpan P80 150 mesh, P80 200 mesh dan P80
270 mesh. Serta variabel tetap pada penelitian yaitu: pH 11, agitasi sebesar 75
rpm, 40% solid, Suhu 25°C dengan waktu pelindian 1, 2, 4, 8 12, 24 dan 48 jam.
Dari penelitian dapat diketahui bahwa pengujian fire assay sampel core
mengandung kadar emas yang relatif rendah yaitu kurang dari 3,65 ppm, dengan
kandungan mineral paling dominan mineral kuarsa (SiO2) sebesar 77,0% pada
pengujian XRD. Hasil analisis mineragrafi menunjukkan mineral sulfida dalam
bentuk pirit, kalkopirit, galena dan sfalerit yang mengindikasikan bahwa bijih
emas Arinem merupakan bijih emas sulfida berkadar rendah. Persen ekstraksi
emas yang didapat meningkat seiring dengan peningkatan konsentrasi goldix yang
digunakan dan diperoleh persen ekstraksi emas tertinggi pada kondisi konsentrasi
1000 ppm yaitu 79,26%. Sedangkan untuk persen ekstraksi emas yang didapat
meningkat seiring dengan peningkatan distribusi ukuran butir yang digunakan dan
diperoleh persen ekstraksi emas tertinggi pada distribusi ukuran butir P80 270
mesh sebesar 80,02%. Sehingga untuk proses ekstraksi emas pada variasi
konsentrasi adalah menggunakan konsentrasi Goldix sebesar 1000 ppm,
sedangkan kondisi optimum untuk proses ekstraksi emas pada variasi distribusi
ukuran butir adalah pada kondisi P80 270 mesh.
Kata Kunci: Florrea Goldix 570, Leaching, Konsentrasi, Distribusi Ukuran
v
ABSTRACT
In the gold processing, mercury and cyanide are gold leaching reagents
that have toxic effects on the environment and living organisms within it. Florrea
Goldix 570 is an environmentally friendly gold and silver leaching reagent that is
expected to replace cyanide. This study aims to analyze the characterization of
gold ore minerals, analyze the influence of reagent concentration and particle size
distribution on the percentage of gold extraction using the Florrea Goldix 570
reagent.
The material used is a vein type with partially oxidized characteristics,
predominantly sulfide, sourced from PT. Antam Tbk. Site Arinem. Gold grade
determination is performed using fire assay, the chemical composition of the ore
is analyzed using ICP, and the carbon and sulfur content is analyzed using LECO
analysis. Determination of dominant mineral composition is done by XRD testing,
and mineragraphy testing is conducted using an optical microscope. The study is
conducted under reagent concentration conditions of 300, 600, and 1000 ppm,
with feed size distributions of P80 150 mesh, P80 200 mesh, and P80 270 mesh, and
The fixed variables in the research are: pH 11, agitation at 75 rpm, 40% solids,
temperature of 25°C with leaching time of 1, 2, 4, 8, 12, 24, and 48 hours.
From the research, it can be known that the fire assay testing of core
samples contains a relatively low gold content, which is less than 3.65 ppm., with
the most dominant mineral being quartz (SiO2) at 77.0% according to XRD
testing. The results of the mineralogical analysis indicate the presence of sulfide
minerals in the form of pyrite, chalcopyrite, galena, and sphalerite, indicating
that the Arinem gold ore is a low-grade gold ore. The percentage of gold
extraction increases with the increase in the concentration of Goldix, and the
highest percentage of gold extraction is obtained at a concentration of 1000 ppm,
which is 79,26%. As for the percentage of gold extraction, it increases with the
increase in particle size distribution, and the highest percentage of gold
extraction is obtained with a P80 270 mesh particle size distribution, which is
80.02%. Therefore, for the gold extraction process at various uses a Goldix
concentration of 1000 ppm, while the optimum condition for gold extraction
process in grain size distribution variations is at P80 condition of 270 mesh.
Keywords: Florrea Goldix 570, leaching, concentration, size distribution

Item Type: Thesis (Other)
Uncontrolled Keywords: Florrea Goldix 570, leaching, concentration, size distribution
Subjects: T Technology > T Technology (General)
Divisions: Faculty of Engineering, Science and Mathematics > School of Engineering Sciences
Depositing User: Eko Yuli
Date Deposited: 04 Aug 2023 03:16
Last Modified: 04 Aug 2023 03:17
URI: http://eprints.upnyk.ac.id/id/eprint/36779

Actions (login required)

View Item View Item